Beijing Found Mechanical & Electrical.Co., Ltd
|
|
| |
| Products |
|
 |
3026 3025 3025B 3025C Phenolic Cotton Cloth Laminated Sheets |
|
|
|

|

|
Click to enlarge image
|
| Phenolic cotton cloth laminated sheets are made of cotton cloth impregnated phenolic resin by processing under heat and pressure. |
|
Product Type
|
Active Standard
|
Performance & Purpose
|
| 3026 |
JB1679-75 |
ãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂMechanical and Electrical applications. |
| 3025 |
JB886-75 |
ãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂMechanical applications. |
| 3025B |
QB |
ãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂperformance is a little lower than 3025. |
| 3025C |
QB |
ãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂperformance is a little lower than 3025B. |
|
| |
|
|
| specification |
|
No.
|
Item
|
Unit
|
Value
|
|
3026
|
3025
|
3025B
|
3025C
|
|
1
|
Density |
g/cm3
|
1.30-1.40
|
1.30-1.40
|
1.30-1.45
|
1.30-1.45
|
|
2
|
Martens heat resistance (LW) |
|
125
|
125
|
125
|
125
|
|
3
|
Flexural strengthãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≥ |
MPa
|
130
|
110
|
90
|
70
|
|
4
|
Tensile strengthãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≥ |
MPa
|
80
|
70
|
—
|
—
|
|
5
|
Impact strengthï¼ÂÂÂÂÂÂÂÂÂÂcharpyãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≥ |
|
30
|
25
|
20
|
15
|
|
6
|
Pressing strengthãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≥ã ã Perpendicular to lamination ã Parallel to lamination |
MPa
|
250 150
|
—
|
—
|
—
|
|
7
|
Water absorption( Thickness 10mm)ãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≤ |
%
|
1.0
|
|
|
|
|
8
|
Adhesion forceãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≥ |
N
|
|
5390
|
4500
|
4500
|
|
9
|
Voltage endurance perpendicular to lamination ãÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ≥ (in oil 90±2âÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂÂ) ã Thicknessï¼ÂÂÂÂÂÂÂÂÂÂ0.5ï½ÂÂÂÂÂÂÂÂÂÂ1mm ã Thicknessï¼ÂÂÂÂÂÂÂÂÂÂ1.1ï½ÂÂÂÂÂÂÂÂÂÂ2mm ã Thicknessï¼ÂÂÂÂÂÂÂÂÂÂ2.1ï½ÂÂÂÂÂÂÂÂÂÂ3mm |
kV/mm
|
—
|
4.0 3.0 2.0
|
— — 2.5
|
— — 2.5
|
|
10
|
Thickness |
mm
|
0.5-100
|
2.0-100
|
|
11
|
Area of the sheets |
mm
|
2040×1020ï¼ÂÂÂÂÂÂÂÂÂÂ1220×1020ï¼ÂÂÂÂÂÂÂÂÂÂ2460×1230
|
|
|
|
|
|
| |
|
|
|